Development of cement boards from coconut shell ash for energy and environment conservation
Abstract
This research aims to develop the cement board from coconut shell ash. The
Portland cement type1: fine sand: tap water ratio is equal to 1: 0.4: 0.33 by weight. The 5
ratios of Portland cement type1: coconut shell ash include 1: 0.12, 1: 0.13, 1: 0.14, 1:
0.15 and 1: 0.16 by weight. The cement board production uses the pressure casting in
normal temperature (30 – 35 degree of Celsius) and controls the 0.75 g/cm3 of density
then test the properties of cement-bonded fiberboard follow TIS 878-2537 standard
(cement bonded particle board: high density). From the results, 1: 0.12 is the most
suitable ratio of cement board from coconut shell ash. This developed cement boards
can reduce the quantity of coconut shell ash waste and have the good thermal
insulation.
Collections