The effect of electrolysis to recovering tungsten carbide
View/ Open
Date
2015-05-19Author
จำนงค์พันธ์, ปฐมพงษ์
วงษ์ศรีษะ, สหรัตน์
บุญกนิษฐ, ปริญญ์
Metadata
Show full item recordAbstract
Recovering of tungsten carbide (WC) with the electrolysis solution in the electrolyte to a reaction with cemented carbide scraps 0.2-1.0 V between temperature from 30-80 C concentration 1-7 N hydrochloric acid solution within 48 hours, the results showed the cemented carbide dissolution proper to the influence of voltage, temperature and solution concentration. Can recovering tungsten carbide, purity over 95.62% of which contain other ingredients include titanium, 1.74% tantalum, 1.68%, and niobium, 0.42% concluded that the electrolysis recovering tungsten carbide is appropriate under voltage is 0.4 V, temperature 80C 7 N solution of hydrochloric acid recovery rate of tungsten carbide powder, about 91.37% with an average particle size of 1.0 m