A study and analysis influence of silver gold copper sing ting alloying element onto mechanical properties and microstructure (specified a colored difference) and anti-tarnish behavior of low gold alloys 8wt% Ag Au Cu Zn Sn
Abstract
This Research is a Development of 8k White Gold low Alloy Metal Components for
Jewelry Pieces. By Study and Analyze the Influence of Silver Alloy, Gold Alloy, Bronze
Alloy, Zinc Alloy and Tin Alloy. Which Affect Microstructure and Mechanical Properties.
(The Different of Color Scales) And Resistance Behavior of Lowered 8k White Gold Alloy
in Varies Ratio.
The Results Showed that Tests and Analysis to Find the Quantities of Elements has
found out that Chemical Components of 8k White Gold Low Alloy Metal had a Little
Different Quantities when Compared Between Before and After Centrifugal Casting
Process. The Tests and Analysis Results of Mechanical Properties of Test Pieces Showed
that the Hardness and Tensile Strength of 8k White Gold Low Alloy Metal with Mixture
of 33.33%Au+50.67%Ag+10%Cu+5%Zn+1%Sn had Minimum Ultimate Tensile Strength
Equal 0.54 kN/mm2, Minimum Elongation Percentage of 55% and Maximum Hardness of
137.0 HV. The Test Results also Show that the Mechanical Properties of the Material are
Brittle Material. When Perform a Forming Process, the Pieces will be Easily Broken which
was Meant that the Forming Process would be Difficult. But The Color Level of the Test
Pieces at this Composite Ratio had the Best Metal Color Level. The Brightness L * = 74.87
was a * = -0.89, b * = 13.74 and the Value of ΔE with the Lowest Color Difference Level
of 1.35. Compared to other Varies Ratio. It Showed that 8k White Gold Low Alloy Metal
Test Pieces were Very Green and Came out Slightly Yellow Compared to the Blue Line
that Approached the Standard Line. These Properties were the Physical Properties
Required in 8k White Gold Low Alloy Metal Jewelry Pieces Production. Also there were
the Results of 8k White Gold Low Alloy Metal in Two Formulas 8k 33.33%Au+50.67%Ag
+8%Cu+7%Zn+1%Sn, 33.33%Au+50.67%Ag+8%Cu+8%Zn+0%Sn. These Formulas had
Tensile Strength in the Range of 1.10, 0.60 kN /mm2, Elongation Percentage in the Range
of 70, 61% and Hardness of 115.6, 123.3HV, Respectively. The Results of the Mechanical
Properties Test of the Test Pieces Showed that 8k White Gold Low Alloy Metal 33.33%
Au+50.67%Ag+8%Cu+7%Zn+1%Sn has Similar Tensile Strength but Maximum Elongation
Percentage of 70% and Minimum Hardness of 115.6HV. Which was Suitable for Forming
Because of good Ductility and Stretchness Properties (Ductile Material). Forming would
be Easy. These were Good Mechanical Properties for Forming Precious Metals.